+ | 17/ | ||
+ | |||
+ | 3D model: cone | ||
+ | |||
+ | * Beeswax 01 (0,8z 7f) | ||
+ | | ||
+ | * bed: 25°C | ||
+ | * result: Prints beautifully. Z-axis skipping (Z-axis motion is too fast). Layers delaminate easily, as they are not fused. | ||
+ | * Beeswax 01 | ||
+ | * nozzle: **40°C** | ||
+ | * bed: 25°C | ||
+ | * result: same as above | ||
+ | * Beeswax 01 | ||
+ | * nozzle **45°C** | ||
+ | * bed: 25°C | ||
+ | * result: flakey / grainy texture, but stronger layer adhesion. | ||
+ | * Beeswax 01 | ||
+ | * nozzle: **50°C** | ||
+ | * bed: 25°C | ||
+ | * result: super flakey | ||
+ | * Beeswax 01 | ||
+ | * nozzle: 50°C | ||
+ | * bed: 25°C | ||
+ | * **warm up time: 15min** | ||
+ | * result: a little more consistent | ||
+ | * Beeswax 01 | ||
+ | * nozzle: 50°C | ||
+ | * bed: 25°C | ||
+ | * warm up time: **40min** | ||
+ | * result: same as above | ||
+ | * Beeswax 01 | ||
+ | * nozzle: **55°C** | ||
+ | * bed: 25°C | ||
+ | * warm up time: **30min** | ||
+ | * result: separated material: half oil, half solid. 3D print has a dripped texture. The tip of the syringe is cooler. The body of the syringe is much hotter. | ||
+ | * Beeswax 02 (1w 0,5z 7f) | ||
+ | * nozzle: **60°C** | ||
+ | * bed: 25°C | ||
+ | * warm up time: **50min** | ||
+ | * result: Almost completely liquid. Too liquid for the nozzle width. | ||
+ | * Beeswax 03 (1w **0,15z** 7f) | ||
+ | * nozzle: **60°C** | ||
+ | * bed: 25°C | ||
+ | * result: Still a little smudgy. Good consistency: | ||
+ | |||
+ | |||
+ | 24/ | ||
+ | * Beeswax 4 (0,6w 0,15z 7f) | ||
+ | * filament: 70°C | ||
+ | * shape: cone | ||
+ | * result: a luer tip with 0,6mm inner diameter cools the wax down too much, resulting in jams and sudden eruptions of hot wax. | ||
+ | *Beeswax 4 (1,18w 0,15z 7f) | ||
+ | * filament: 70°C | ||
+ | * shape: cone | ||
+ | * result: OK, but printing too slow: cools down too fast | ||
+ | *Beeswax 4 (1,18w 0,15z **20f**) | ||
+ | * filament: 70°C | ||
+ | * shape: cone | ||
+ | * result: Material flow stops. There is a weird buzz which I think is an unprime event. | ||
+ | *Beeswax 4 (1,18w 0,15z 20f) | ||
+ | * filament: 70°C | ||
+ | * shape: cone | ||
+ | * **head control**: unprime set to zero | ||
+ | * result:? | ||
+ | * Beeswax 5 | ||
+ | * filament: 35°C | ||
+ | * shape: vessel v1 | ||
+ | * result: layers too thick, had to change material flow rate multiplier to 1.5. |